I have never seen polymer parts require gas out time so if you stick it in the oven and don’t see any oil bleeding against the matte blasted look in about 30 min I’d rock and roll with coating after it cooled down.

 

For polymer parts I acetone wash then blast at 90-100psi and bake at 180degrees for 2 hours and let them fully cool down before handling 

 

Be sure when you hang polymer parts you aren’t putting much pressure is any direction (i.e. dont loop hanger thru Glock base pad track and then once it’s cured it’s dimensions are opened up causing it to be loose)

 

good luck 

Edited by Hawk21
Link to comment
Share on other sites

  • 3 weeks later...

I did it at 150 for 2 hours. I figured that's not to hot for most polymer and that's what I have seen for Oakley sunglasses . I did blast it lightly and wiped it off with brake cleaner. 

 

Before is the black handle after is the red

 

IMG_0783.jpg

IMG_2182.HEIC

Edited by Bmans45
Link to comment
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

 Share

×
×
  • Create New...